- 1. Durability overview
- 2. Drivers of durability
- 3. IS 456:2000 durability criteria (Table 5)
- 4. Durability test categories
- 5. Key lab tests and targets
- 6. Field and NDT tests
- 7. Advanced indicators
- 8. Routine QA/QC at site
- 9. Durability enhancement actions
- 10. Troubleshooting
- 11. Quick interpretation matrix
- 12. Reference standards
- 13. Consultant checklist
- Disclaimer
Purpose: consultant-ready durability and testing reference. Jump to exposure criteria, lab tests, NDT, QA actions, and acceptance bands using the TOC.
1. Durability overview
Durability is the structureās resistance to environmental and chemical attack while maintaining serviceability. Strength measures capacity; durability governs service life.
2. Drivers of durability
Category | Parameters | Effect |
Material quality | Cement chemistry, SCMs, aggregate reactivity | Permeability and early strength |
Design | W/c, cover, compaction, curing | Microstructure and crack control |
Exposure | Marine, industrial, freezeāthaw, sulphate | Chemical aggressiveness |
Execution | Mixing, vibration, curing regime | Defect and pore structure |
Maintenance | Coatings, waterproofing | Service life extension |
3. IS 456:2000 durability criteria (Table 5)
Exposure | Environment | Max w/c | Min cement (kg/m³) | Min grade | Nominal cover (mm) |
Mild | Dry interiors | 0.55 | 300 | M20 | 20 |
Moderate | Urban | 0.50 | 300 | M25 | 30 |
Severe | Coastal and wet | 0.45 | 320 | M30 | 45 |
Very severe | Aggressive soil | 0.45 | 340 | M35 | 50 |
Extreme | Marine/chemical | 0.40 | 360 | M40 | 75 |
4. Durability test categories
Category | Objective | Common tests | Standards |
Permeability/porosity | Ingress resistance | Water penetration, RCPT | IS 3085, ASTM C1202 |
Chemical attack | Resistance to sulphates/chlorides/carbonation | pH, chloride diffusion, carbonation depth | IS 516, NT Build 443 |
Physical weathering | Thermal and moisture cycling | Freezeāthaw, drying shrinkage | ASTM C666, IS 516 (Pt 5) |
Mechanical integrity | Soundness | UPV, rebound, pull-out | IS 13311 |
Surface integrity | Crack detection | Crack gauge, dye | BS 1881, ASTM C597 |
5. Key lab tests and targets
Test | Standard | Purpose | Typical durable value |
Water penetration | IS 3085 | Depth at 5 bar | ⤠20 mm |
RCPT | ASTM C1202 | Charge passed | < 1000 C |
Chloride diffusion | NT Build 443 | Diffusion coefficient | ā 1Ć10ā»Ā¹Ā² m²/s |
Sorptivity | ASTM C1585 | Capillary intake | < 0.05 mm/min¹/² |
Carbonation depth | RILEM CPCā18 | Phenolphthalein | < 10 mm at 1 year |
Sulphate attack | IS 12330 | Expansion/mass change | < 0.1% expansion |
ASR | IS 2386 (Pt 7) | Reactivity of aggregates | Innocuous only |
6. Field and NDT tests
Test | Code | Purpose | Interpretation |
Rebound hammer | IS 13311 (Pt 2) | Surface hardness | ±15% of actual strength |
UPV | IS 13311 (Pt 1) | Homogeneity/voids | > 4.5 km/s excellent |
Pull-out | ASTM C900 | Bond strength | 1.5ā3 MPa typical |
Cover meter | BS 1881 | Cover check | Per IS 456 |
Half-cell potential | ASTM C876 | Corrosion activity | < -350 mV likely corrosion |
Crack width | ā | Serviceability | < 0.3 mm RCC, < 0.1 mm water-retaining |
7. Advanced indicators
Indicator | Description | Test |
Electrical resistivity | Ion movement resistance | Wenner probe |
Chloride migration (Dcl) | Clā» transport | NT Build 492 |
Permeable voids | Pore volume | ASTM C642 |
Shrinkage/creep | Dimensional stability | IS 516 (Pt 6) |
RCM (rapid migration) | Charge transfer at 60 V DC | EN 12390ā18 |
8. Routine QA/QC at site
Test | Frequency | Equipment | Acceptance |
Slump | Every truck | Slump cone | ±25 mm |
Temperature | Every load | Thermometer | < 32°C |
Compressive strength | Every 50 m³ | Cube molds | ℠fck |
Density | Daily | Scale | ±3% |
Cube density | Weekly | Density test | 2350ā2500 kg/m³ |
Air content | As needed | Pressure meter | < 5% for dense concrete |
9. Durability enhancement actions
Issue | Action | Material/system |
High permeability | Lower w/c | Silica fume, densifier |
Carbonation risk | Improve curing, adequate cover | Anti-carbonation coating |
Chloride ingress | 30ā50% SCM replacement | Slag, fly ash, metakaolin |
ASR | Low-alkali cement | Lithium admixture |
Surface dusting | Correct curing | Lithium densifier/sealer |
10. Troubleshooting
Quick view of failures and fixes
Symptom | Cause | Action |
Plastic shrinkage cracks | Rapid evaporation | Wind breaks, early curing, fibres |
Efflorescence | Permeability and curing | Improve curing, breathable coatings |
Rust staining | Rebar corrosion | Half-cell assessment, inhibitors |
Low UPV | Honeycombing | Core tests, microconcrete repair |
High carbonation | Thin cover/porous matrix | Increase cover, anti-carbonation coat |
11. Quick interpretation matrix
Test | Unit | Durable range | Quality grade |
RCPT | C | < 1000 | Excellent |
Water penetration | mm | < 20 | Excellent |
Carbonation depth | mm | < 10 | Good |
UPV | km/s | > 4.5 | Excellent |
Halfācell | mV | > ā250 | Safe |
Resistivity | kΩ·cm | > 20 | Durable |
Chloride diffusion | m²/s | < 1Ć10ā»Ā¹Ā² | Durable |
12. Reference standards
Code | Description |
IS 456:2000 | Durability and design |
IS 10262:2019 | Mix design guidance |
IS 516 (Pt 5ā6):2021 | Durability and shrinkage |
IS 3085:1965 | Water permeability |
IS 13311:1992 | NDT methods |
ASTM C1202, C876 | RCPT and corrosion |
EN 12390ā8 | Water penetration |
RILEM CPCā18 | Carbonation |
NT Build 443 / 492 | Chloride tests |
13. Consultant checklist
- Test for both strength and durability; do not assume one guarantees the other.
- Select SCMs to meet durability targets and exposure class.
- Specify coatings or crystalline waterproofing where permeability risk is high.
- Schedule periodic NDT for long-term monitoring.
- Keep all test data in a digital QA sheet for traceability.
Disclaimer